For many valve engineers worldwide, quality concern over Chinese Alloy 718 material exists for a long time. Over a series of case stories, ECA will show you the remarkable progress of China’s nickel alloy industry.
Our first case focuses on the Laves phase in Alloy 718 (UNS N07718) under API 6ACRA, the core specification for age-hardened CRA materials for wellhead and valve components. One non-negotiable metallurgical requirement is clearly stated: the micro-structure shall be free from Laves phase.
What is Laves phase?
Niobium delivers the primary strengthening effect in Alloy 718. During solidification, γ nickel matrix dendrites form first and reject Nb into the remaining interdendritic liquid. Once local Nb enrichment reaches the critical level, a non-equilibrium terminal eutectic reaction takes place:L →γ + Laves, forming brittle, Nb-rich Laves intermetallics.
What risk does Laves phase bring to materials service?
Laves phase is inherently brittle. Interfaces between Laves and the γ matrix act as crack initiation sites. Under cyclic pressure, erosion, H₂S and hydrogen charging, cracks propagate rapidly along interdendritic networks, causing seal leakage or catastrophic fatigue failure.
From ECA's view, leading Chinese superalloy mills launched targeted development programs for API 6ACRA grade 718 forgings and valve flat bars around 2018.
How do we do to deliver quality materials?
During ECA's discussion with our partner mills, we find there are 4 aspects around the 4 processes from VIM to ESR to VAR to homogenization.
This particle, we will describe the issues in VIM process.
-Sulphur, phosphorus, boron and silicon act as accomplices: even minute amounts of boron and phosphorus depress the melting point of interdendritic liquid, extending the residence time of residual liquid and aggravating eutectic Laves formation. At ECA's supply record, Sulphur is now steadily controlled at the 0.001% level.
-Aluminium and titanium govern the precipitation sequence of carbides. Controlled preferential precipitation of MC (NbC) sequesters a portion of niobium in advance, reducing the quantity of niobium partitioning into the eutectic liquid phase. However, excess levels will trigger the formation of other brittle phases.
As ECA, we supply this qualified Alloy718 flat bars for valve applications with full documentation, verifiable metallurgy and certified UT performance, compliant with API 6ACRA for valve plates and seats for domestic and export valve OEMs.
Do you have quality concerns when importing Chinese Alloy 718 material for oil & gas application?
What is the difference between API 6A CRA, AMS 5662 and AMS 5663? All three standards define material requirements for Alloy 718. AMS 5662 and AMS 5663 cover Alloy 718 for aerospace engine service, not imposing mandatory requirements for sour-service resistance, transverse Charpy impact. AMS 5662 specifies Alloy 718 supplied in the solution-annealed condition, whereas AMS 5663 covers material delivered in the solution-annealed and age-hardened condition. API 6A CRA governs Alloy 718 for sour-service oil and gas wellhead applications. It is tailored for pressure-containing and pressure-controlling components used on wellheads and Christmas trees under sour oil and gas service (H₂S, Cl⁻), and aligns with NACE MR0175 / ISO 15156.
How does the cooling methods influence Alloy 718 material’ performance in oil & gas sector?
What is the difference between Alloy 718 and Alloy 725?