Corrosion resistant alloys

Alloy C-276

Alloy C-276

Alloy C276 is applicated for sulfur and chloride-bearing environments.


Description
Chemical Compositions
Applications
Technical Standards
Product Forms
FAQ



UNS Number

UNS N10276

Industry Name
Alloy C-276, NC15D14KFe, W.Nr.2.4819, Hastelloy® C-276

Product Forms

Bars, Wires, Plates, Strips, Forgings


General Characteristics

Alloy C-276 is engineered to survive the harshest mixed-corrosion service conditions where most stainless steels and standard nickel alloys fail.

Unlike conventional stainless steel, it remains stable under mixed oxidizing-reducing acids, wet chlorine and chloride-rich brines, resisting pitting, crevice attack and stress corrosion cracking. 

Its low-carbon formulation avoids intergranular corrosion after welding or laser melting. 

As spherical powder for SLM additive manufacturing, it delivers consistent corrosion resistance for complex custom components operating in aggressive corrosive service.






Chemical compositions of UNS 10276

Co

W

Cr

Mo

Fe

Mn

Si

P

S

V

C

Ni

≤2.5

3.0-4.5

14.5-16.5

15.0-17.0

4.0-7.0

≤1.0

≤0.08

≤0.04

≤0.03

≤0.35

≤0.010

Bal.




Specific Chemical Compositions Function

  • Molybdenum provides resistance to pitting, crevice corrosion and chloride stress corrosion cracking whileas stabilizing the passive film in reducing acid environments.

  • Chromium delivers oxidation resistance and passive film protection in oxidizing media such as nitric acid and hot oxidizing brines.

  • Low carbon content minimizes intergranular carbide precipitation during high‑temperature processing or welding, preserving corrosion resistance in heat‑affected zones.

  • Nickel offers ductility, toughness and resistance to chloride‑induced stress corrosion cracking, good fabricability and weldability.


Chemical processing||Heat exchanger tubes|Reactor vessels, reactor liners|Control valve bodies|Distillation column trays
Oil & gas / sour service||Choke valve parts, wellhead components|Subsea instrument housings|Manifold components
Flue gas desulfurization (FGD)||Ductwork dampers|Scrubber internals|Spray nozzles|Mist eliminators
Additive manufacturing|| Corrosion-resistant valve bodies|Micro-flow control nozzles|Small sour-gas sensor holders


Technical specifiactions of Alloy C276 

Technical Standards

Product Form

ASTM B574

Rod

ASTM B564

Forgings

ASTM B575

Plate, Sheet and Strip

ASTM B619

Pipe

ASTM B622

Pipe and Tube

    

   




Product forms of Alloy C276 ECA provides 

Product form

Size range (mm)

Forged bar

Dia.70-500

Rolled bar

Dia.2.0-70

Flat bar

T4-50*W60-300

Wire

Dia.0.25-18.0

Forged ring

OD 30-350* ID 30-350

Strip

0.15-3.0 * 20-200

Plate

1-25 * ≤1200 * ≤1200

Seamless tube

OD 6.0-200 * 0.6-20


1. Is alloy C-276 magnetic?

No.


2. Is alloy C-276 active to galvanic corrosion?

No. It is passive to galvanic corrosion.


3. Alloy C-276 coefficient of thermal expansion?

θ/°C

20-100

20-200

20-300

20-400

20-500

20-600

20-700

20-800

α

12.2

12.4

12.9

13.2

13.5

13.6

14.1

14.8


4. Alloy C-276 thermal conductivity?

θ/°C

-168

-73

20

25

100

200

300

400

500

600

700

800

900

1000

1100

W/(m·°C)

7.2

8.7

9.8

/

11.2

12.8

14.7

16.4

18.2

20

21.9

23.7

25.4

27

28.3


5. Alloy C-276 young's modulus?

θ/°C

25

100

200

300

400

500

600

700

800

900

1000

Gpa

205

203

198

192

186

180

178

167

159

150

141


6. Alloy C-276 is prone to hydrogen embrittlement?

Hastelloy C-276 also suffers hydrogen embrittlement, especially in the thermally aged condition when it loses its solution-annealed ductility. It has been found that Hastelloy C-276 is more prone to hydrogen embrittlement than alloy 625 and stainless steel 316L.


Leave your comment
Leave Your Message